PERBOND
← The Journal
· The PerBond Team

Bonding Sheet Metal: Why a Longer Overlap Stops Adding Strength

Thin sheet metal is where adhesive bonding earns its place: it joins panels without the heat distortion of welding, seals the seam as it goes, and spreads load along a line instead of concentrating it at spots. It is also where the most common mistake in bonded design shows up most clearly, which is assuming that a joint twice as long is twice as strong. This guide uses the Lap Joint Efficiency Calculator to show what happens along an overlap in 1 mm steel and aluminium, and what to change when a joint needs to carry more.

Read this first

The figures here illustrate a principle. They are not strength ratings and they are not a repair method. Never use them, or any calculator on this site, to design or repair structural parts of a vehicle (chassis, sills, pillars, crash structure, suspension and seat-belt mountings) or anything else load-bearing, overhead or safety-critical. Vehicle body repairs must follow the vehicle manufacturer's repair procedure with the adhesive it specifies. Other critical joints need a qualified engineer and tested design values.

What happens inside a loaded overlap

Picture two strips bonded with an overlap and pulled in opposite directions. Each strip carries the whole load where it enters the joint and none at its free end, having handed the load across to the other strip through the adhesive along the way. So each strip is stretched most at one end of the overlap and not at all at the other, and the two strips are stretched at opposite ends.

The adhesive between them has to absorb that mismatch. At each end of the overlap, one strip has stretched and the one facing it has not, so the adhesive there is sheared hard. In the middle, both strips have stretched by similar amounts and the adhesive is barely strained. The result is a shear stress that peaks at both ends and sags in between. The joint starts to fail when the ends reach the adhesive's limit, however little the middle is doing.

This was first analysed by Volkersen in 1938, and his model is what the calculator runs. It reports two things: the peak shear divided by the average, and the "elastic efficiency", which is the fraction of the simple strength-times-area figure the joint reaches when the ends hit their limit.

The numbers for 1 mm sheet

The table uses the calculator's defaults for the adhesive (shear modulus 1,000 MPa, bond line 0.2 mm) and its built-in stiffness values for steel (210 GPa) and aluminium (70 GPa).

Overlap1 mm steel: efficiency1 mm steel: peak ÷ average1 mm aluminium: efficiency2 mm aluminium: efficiency
10 mm73%1.37×51%65%
15 mm57%1.77×35%48%
20 mm45%2.24×26%37%
25 mm36%2.75×21%30%
40 mm23%4.37×13%19%
60 mm15%6.55×9%12%

Three patterns are worth taking from it.

  • Efficiency falls as the overlap grows. On 1 mm steel it goes from 73 percent at 10 mm to 15 percent at 60 mm. Each added millimetre is worth less than the one before.
  • Stiffer sheet shares the load better. Steel is 3 times as stiff as aluminium, stretches less, and shows a higher efficiency at every overlap.
  • Thicker sheet does too. 2 mm aluminium sits above 1 mm aluminium in every row, because a thicker strip stretches less under the same load.

What that does to the load a joint carries

Efficiency falling is not the same as strength falling. A longer joint has more area; the question is whether the extra area is used. Take a strip 25 mm wide in 1 mm steel with a 20 MPa adhesive, and compare the straight-line figure (area times strength, no safety factor, from the Bond Strength Calculator) with the same figure multiplied by the elastic efficiency:

OverlapStraight-line figureElastic efficiencyElastic-model figure
12.5 mm6,250 N64%4,020 N
25 mm12,500 N36%4,544 N
50 mm25,000 N18%4,582 N

The straight-line column doubles each time the overlap doubles. The elastic-model column barely moves: going from 25 mm to 50 mm adds about 1 percent. On this model the joint has reached a plateau. The ends are carrying what they can, and the extra bonded metal in the middle is along for the ride.

The calculator flags the point where this sets in. Once the overlap is more than 20 times the sheet thickness, it reports that length has stopped helping: that is 16 mm for 0.8 mm sheet, 20 mm for 1 mm, and 40 mm for 2 mm. On 1 mm steel the 25 mm row in the first table is already past it (flagged: yes), while 20 mm is not (flagged: no).

How literally to take these figures

Not very, and the calculator says so itself. The model is elastic: it assumes the adhesive behaves like a perfect spring right up to failure. Structural adhesives do not. The tough, modern ones yield at the overstressed ends, stop taking more load there and pass it inward, so a real joint keeps gaining strength for longer than the table suggests and ends up well above the elastic figure. A brittle adhesive behaves much more like the model.

The published strength of an adhesive already includes some of this. The standard lap-shear test uses a 12.7 mm overlap on 1.62 mm aluminium. By the same elastic model that coupon is at 51 percent efficiency with a peak 1.97 times the average, and the data-sheet figure is the average stress at which it broke. So the data-sheet number is not a pure material property; it is the result for one short, standard joint.

What the elastic figures are reliable for is direction. They are right that the ends do the work, right that long overlaps waste adhesive, and right about which changes help.

What to change instead of length

  • Width. A wider joint is more joint, with the same stress pattern repeated across it. Double the width and the capacity doubles on any model. On sheet metal this is usually free: bond the whole flange, not a strip of it.
  • A thicker bond line, within the data sheet's range. A thicker layer of adhesive is more compliant and spreads the load. At a 25 mm overlap on 1 mm steel the elastic efficiency is 26 percent with a 0.1 mm bond line, 36 percent at 0.2 mm and 54 percent at 0.5 mm. Bond-line thickness also affects the adhesive's own strength, so stay inside the manufacturer's limits; many panel adhesives contain glass beads to set it.
  • A tougher adhesive. Toughened epoxies and structural acrylics are designed to yield at the ends without cracking. This is the main reason they outperform rigid adhesives on sheet metal even when their headline strength is similar.
  • Fillets and tapered ends. Leaving the squeezed-out fillet at the end of the overlap, or thinning the sheet edge, lowers the stress peak.
  • Combining methods. Rivets, clinch points or spot welds through a bonded seam resist peel at the ends and hold the parts while the adhesive cures.

The load the calculator does not see: peel

A single lap in thin sheet is offset, so pulling on it makes the sheets bend and tries to lever the ends of the joint open. That opening load is called peel, and adhesives resist it far less well than shear. In thin sheet, peel at the ends is usually what starts a failure, well before the shear figure is reached. It is why bonded sheet-metal seams are designed as folded hems and flanges that keep the adhesive in shear and compression, and why a seam that might see peel gets fasteners at its ends. The efficiency calculator models shear only.

What the calculator does not cover

  • Peel and bending, which govern most thin-sheet joints.
  • Yielding of the adhesive or the metal. The result is elastic and pessimistic.
  • Two different sheets. It assumes both are the same material and thickness.
  • Fatigue, impact, heat, moisture and corrosion under the bond.
  • Surface condition. Oil, zinc coatings, primers and paint all change what the bond actually reaches.

To size an overlap from a load, use the Lap Joint Designer; this guide works three cases through.

Safety and limits

Panel-bonding and structural adhesives are hazardous until cured. Epoxy resins and hardeners are skin sensitisers. Two-part acrylics give off strong, flammable vapour. Polyurethane adhesives and seam sealers contain isocyanates, which can cause asthma. Wear nitrile gloves and eye protection, work with good ventilation, wash with soap and water and never solvent, and read the Safety Data Sheet (SDS) first.

Heat is a specific hazard on bonded metal: welding, grinding or flame-cutting near cured adhesive, sealer or foam releases toxic fumes and can start a fire inside a closed section. Remove the adhesive from the heated area first, and ventilate.

Follow the adhesive manufacturer's preparation, mix ratio and cure schedule exactly. And once more: nothing here qualifies a bonded joint for a vehicle structure or any load-bearing use. That takes the manufacturer's procedure, tested values and a qualified engineer.

Get new guides by emailOccasional emails. No spam. Unsubscribe anytime.